본 시험은 ㈜연진에스텍의 Texture Analyzer (모델 TXA™-Micro-Precision)을 이용해 Compression mode에서 0.1 mm/sec 속도로 hydrogel 샘플을 압축시험하여 Stress/Strain에 의한 Young’s Modulus와 ΔStress/ΔStrain에 의한 Tangential Modulus를 측정 분석하였다.
Strain-Stress curve of sample #1
|
Max. Stress (kPa) |
Max. Strain |
Max. Modulus ( kPa) |
Tangential Modulus ( kPa) |
Sample #1 |
1.67 |
0.3 |
5.61 |
7.60 |
Strain-Stress curve of sample #2
|
Max. Stress ( kPa) |
Max. Strain |
Max. Modulus ( kPa) |
Tangential Modulus ( kPa) |
Sample #2 |
0.30 |
0.4 |
0.89 |
0.79 |
Strain-Stress curve of sample #3 & 4
|
Max. Stress ( kPa) |
Max. Strain |
Max. Modulus ( kPa) |
Tangential Modulus ( kPa) |
Sample #3 |
532.35 |
0.15 |
3578.81 |
3674.23 |
Sample #4 |
1556.77 |
0.15 |
10459.92 |
10743.08 |